Hydrogen embrittlement in a PEM water electrolyzer is less a bulk-material problem than an interface and operating-environment problem. At the cathode, hydrogen is generated directly on and around the components that conduct current and support the membrane electrode assembly. Where that hydrogen can enter titanium, it may accumulate at susceptible sites, precipitate as titanium hydride and promote cracking. Reducing the risk therefore means designing the cathode material, its surface protection, the mechanical loading and the validation plan as one system.
The two electrodes of a PEM water electrolyzer operate in very different environments. The anode combines low pH, high potential and oxygen evolution, which is why noble-metal-coated titanium is the state of the art for anode porous transport layers (PTLs) [1, 2]. The cathode operates at low potential in a reducing, hydrogen-rich atmosphere. Carbon corrosion is not a concern there during operation, and carbon-based gas diffusion layers (GDLs) made from felts, papers or woven substrates are widely used [1, 2]. A material selected for anode corrosion resistance is therefore not automatically the best answer to cathode hydrogen exposure.
Titanium offers corrosion resistance, low density and established compatibility with PEM hardware, but it has a high affinity for hydrogen and is a typical hydride former [4]. Because the hexagonal α phase of commercially pure titanium dissolves very little hydrogen at ambient temperature, hydrides can form at comparatively low hydrogen contents. Classical corrosion literature associates significant hydriding of titanium with very low or very high pH, temperatures above roughly 80 °C and an available hydrogen source [3]. The PEM cathode is acidic and hydrogen-rich by design; hot, pressurized operation moves it closer to the remaining condition. For titanium bipolar plates, studies summarized in a recent review report mechanical failure above about 8,000 ppm hydrogen and uptake of more than 1,000 ppm within 500 h of operation [1].
This does not mean that every titanium cathode component will fail. It means the risk depends on hydrogen activity, temperature, pressure, surface condition, microstructure, residual and applied stress, and exposure time — and that a robust cathode design accounts for these factors from the outset.
The damage sequence can be described in five connected stages (Figure 1):
Hydrogen is generated. Protons are discharged at the cathode (H+ + e− → Hads), producing adsorbed hydrogen on the catalyst and on nearby conductive surfaces.
Most hydrogen recombines and leaves. Adsorbed atoms combine to H2 and exit through the pore network — the intended pathway.
A fraction enters the metal. Where titanium is exposed — at coating pinholes, internal pores, cut edges or worn contact points — some adsorbed hydrogen is absorbed instead of recombining.
Hydrogen is trapped and precipitates as hydride. Absorbed hydrogen diffuses through the lattice and concentrates at grain boundaries, phase boundaries and stressed regions. Atom-probe studies have observed titanium hydrides along α grain boundaries and α/β phase boundaries [4]. The α-to-hydride transformation is accompanied by a volume expansion that creates a local stress field around the hydride [5].
Cracks initiate and grow. In grade 2 titanium, high hydrogen contents lead to failure by hydride cleavage, whereas moderate contents already reduce ductility through hydrogen-enhanced localized plasticity, before hydrides form [6]. In a porous component this can appear as broken fibers, particle shedding or a progressive loss of contact.

Figure 1. Schematic of hydrogen ingress and hydride-assisted damage at a titanium cathode PTL. (a) Cell-level cross-section: proton exchange membrane (PEM), cathode catalyst layer (CL), Ti PTL and bipolar plate (BPP); the dashed box marks the region enlarged in (b). (b) Surface and grain-scale mechanism: (1) proton discharge to adsorbed hydrogen; (2) recombination to H2; (3) absorption at a coating defect and diffusion into α-Ti; (4) hydride precipitation at trapping sites under applied or residual stress (σ); (5) crack initiation and growth through the hydride-rich zone. Conceptual illustration; not to scale.
A porous transport layer provides electrical contact, water and gas pathways, and mechanical support. The same features can intensify hydrogen-assisted damage. A large internal surface area offers many potential entry sites. Fiber intersections, sintering necks and sharp geometric transitions concentrate stress, and the alternating rib–channel pattern of the bipolar plate produces non-uniform compression. A complex three-dimensional pore network is also far harder to coat continuously than a flat coupon.
A coating that looks acceptable on the outer surface may therefore leave vulnerable internal regions. Cross-sectional inspection, edge-coverage checks and tests on representative porous samples are more informative than a single top-surface measurement.
Hydride is not harmful in every form. A thin subsurface TiHx layer produced by acid etching has been used on anode titanium diffusion layers to limit passivation and lower contact resistance [1, 3]. What matters is the amount, location and morphology of hydride relative to stress — not its mere presence.
Where stack pressure, mechanical support and transport requirements allow, carbon paper or felt removes titanium from the hydrogen-evolving interface altogether, at significantly lower cost than coated titanium [2]. Recent cell-level work provides practical guidance for this choice [2]:
A microporous layer (MPL) gave only a slight benefit with a conventional high-loading CCM, but substantially reduced ohmic, kinetic and residual overpotentials at an ultra-low cathode loading of 0.054 mgPt cm−2.
Carbon fibers cannot penetrate the oxide on an uncoated titanium flow field, which leads to high ohmic resistance; coated or highly conductive flow fields are recommended when carbon GDLs are used.
Adding 5 wt% PTFE to the GDL increased ohmic resistance without improving performance.
Carbon media must still be qualified for compression, creep, contact resistance and differential pressure. They should not be transferred to the oxygen-evolving anode without a separate corrosion assessment.
Some cathode architectures still require titanium for mechanical, dimensional, integration or pressure reasons. In that case the surface system must restrict hydrogen access to the substrate while keeping contact resistance low. A recent review outlines several barrier concepts [1]:
Gold can limit hydrogen absorption, but a relatively thick coating (>200 nm) is reported to be necessary.
Pinhole-free carbon coatings have been shown to reduce hydrogen absorption, though cost and processing remain obstacles.
Native oxide plus gold dots: the oxide limits hydrogen entry while gold dots covering less than 10 % of the surface provide sufficient electrical contact.
The key word is continuous. A thin coating with pores, cracks, damaged edges or incomplete coverage of internal pores can show excellent contact resistance in a laboratory test while still allowing localized hydrogen ingress. Coating qualification should therefore cover thickness distribution, continuity, adhesion, defect mapping and edge coverage — not only an average thickness.
Platinum deserves a specific caution. Pt coatings are widely used on titanium PTLs and bipolar plates to prevent passivation [1], but hydrogen can absorb in platinum, and embrittlement has been reported to occur even under Pt coatings [1]. Pt should not be assumed to block hydrogen; its suitability must be demonstrated at the intended hydrogen pressure, temperature and duty cycle.
The oxide trade-off applies more generally: a thicker or more stable surface oxide slows hydrogen entry but raises interfacial contact resistance [1]. The final choice should rest on cell-level data, not on a coating name.
Hydrogen and mechanical stress reinforce each other. Uniform stack compression avoids highly loaded fiber contacts and local bending. Rounded features, controlled pore morphology and adequate support under bipolar-plate ribs reduce stress concentrations. Cut edges and joining regions should be treated as functional surfaces, because they can carry high stress while exposing fresh titanium.
Operating conditions matter just as much. Higher hydrogen pressure, elevated temperature, long hold periods and repeated start–stop or load cycling all change hydrogen uptake and crack-growth behavior. Accelerated tests are useful only if they preserve the relevant mechanism: a short coupon test at ambient pressure cannot represent a pressurized, compressed porous component in an operating stack.
A robust validation program links surface quality to material condition and cell performance (Figure 2):
Surface and coating verification. Measure thickness distribution and contact resistance; inspect internal pores, cross-sections, cut edges and likely wear locations for discontinuities.
Hydrogen uptake and hydride detection. Quantify hydrogen content (e.g. inert-gas fusion) and, where needed, use thermal desorption spectroscopy (TDS), X-ray diffraction and electron microscopy (SEM/EBSD) to locate hydrogen accumulation and hydrides.
Mechanical comparison before and after exposure. Track compression response, bending or tensile behavior, microcracking, fiber breakage and particle shedding.
Electrochemical and electrical monitoring. Follow interfacial contact resistance (ICR), cell voltage, high-frequency resistance (HFR) and impedance (EIS) during long-duration and cycling tests.
Failure analysis. Correlate cracks or powdering with coating defects, pore geometry, rib–channel loading and local operating conditions to identify whether the dominant lever is material, coating, mechanics or operation.

Figure 2. Design and qualification hierarchy for reducing hydrogen embrittlement risk at the PEM cathode: (i) material selection by electrode environment; (ii) barrier and mechanical design where titanium is retained; (iii) qualification under representative operating conditions, with failure analysis feeding back into earlier decisions. Barrier concepts after [1]; carbon GDL guidance after [2].
Hydrogen embrittlement risk cannot be controlled by specifying only a titanium grade or a nominal coating thickness. The most reliable hierarchy is to choose materials by electrode environment; to avoid titanium at the cathode wherever a qualified carbon medium meets the requirements; and, where titanium is unavoidable, to use a verified continuous barrier. Mechanical design and representative durability testing complete the strategy.
YIANTENG was founded in 1993 and has 33 years of experience in electrode and coating technology. We work with customers to evaluate substrate, surface preparation, coating architecture, contact behavior and operating conditions together, so that material decisions reflect how the electrolyzer is actually assembled and operated.
To discuss a cathode diffusion-layer or coated-titanium application, visit www.yat-electrode.com.
[1] C. Wang, J. M. Stansberry, R. Mukundan, et al., Proton exchange membrane (PEM) water electrolysis: cell-level considerations for gigawatt-scale deployment, Chem. Rev. 125 (2025) 1257–1302. https://doi.org/10.1021/acs.chemrev.3c00904
[2] N. Hensle, J. Hoffmann, Z. Najafianashrafi, T. Smolinka, P.-Y. A. Chuang, A. Weber, Understanding the use of carbon-based porous transport layers at the cathode in PEM water electrolysis, J. Power Sources 642 (2025) 236913. https://doi.org/10.1016/j.jpowsour.2025.236913
[3] T. Bystron, M. Vesely, M. Paidar, et al., Enhancing PEM water electrolysis efficiency by reducing the extent of Ti gas diffusion layer passivation, J. Appl. Electrochem. 48 (2018) 713–723. https://doi.org/10.1007/s10800-018-1174-6
[4] Y. Chang, A. J. Breen, Z. Tarzimoghadam, et al., Characterizing solute hydrogen and hydrides in pure and alloyed titanium at the atomic scale, Acta Mater. 150 (2018) 273–280. https://doi.org/10.1016/j.actamat.2018.02.064
[5] J. Kim, E. Plancher, C. C. Tasan, Hydrogenation-induced lattice expansion and its effects on hydrogen diffusion and damage in Ti–6Al–4V, Acta Mater. 188 (2020) 686–696. https://doi.org/10.1016/j.actamat.2020.02.029
[6] L. Deconinck, X. Lu, D. Wang, R. Johnsen, K. Verbeken, T. Depover, Multiscale evaluation of hydrogen-assisted mechanical degradation in grade 2 titanium, J. Alloys Compd. 983 (2024) 173959. https://doi.org/10.1016/j.jallcom.2024.173959